Fabrication and Photoluminescence Studies of Tin-Vacancy Centers in Chemical Vapor Deposition Diamond
Rani Mary Joy, Miquel Cherta Garrido, Omar J. Y. Harb, Hendrik Jeuris, Rozita Rouzbahani, Jan D’Haen, Stéphane Clemmen, Dries Van Thourhout, Danny E. P. Vanpoucke, Paulius Pobedinskas, Ken Haenen
Group IV color centers in diamond are promising single-photon emitters for quantum information processing and networking. Among them, the tin-vacancy (SnV) center stands out due to its long spin coherence times at cryogenic temperatures above 1 K. While SnV centers have been realized using various fabrication routes, their in situ formation via microwave plasma-enhanced chemical vapor deposition (MW PE CVD) remains relatively unexplored. In this study, SnV centers, identified by a zero-phonon line (ZPL) near 620 nm, were synthesized in nanocrystalline diamond and free-standing microcrystalline diamond using tin oxide (SnO 2 ) as a dopant source at substrate temperatures of 750°C and 850°C. Photoluminescence measurements reveal that lowering the substrate temperature enhances both the ZPL intensity and spatial uniformity of SnV centers. These results highlight substrate temperature as a key parameter for controlling SnV incorporation during MW PE CVD growth and provide insights into optimizing fabrication strategies for diamond-based quantum technologies.
Group IV color centers in diamond are promising single-photon emitters for quantum information processing and networking. Among them, the tin-vacancy (SnV) center stands out due to its long spin coherence times at cryogenic temperatures above 1 K. While SnV centers have been realized using various fabrication routes, their in situ formation via microwave plasma-enhanced chemical vapor deposition (MW PE CVD) remains relatively unexplored. In this study, SnV centers, identified by a zero-phonon line (ZPL) near 620 nm, were synthesized in nanocrystalline diamond and free-standing microcrystalline diamond using tin oxide (SnO 2 ) as a dopant source at substrate temperatures of 750°C and 850°C. Photoluminescence measurements reveal that lowering the substrate temperature enhances both the ZPL intensity and spatial uniformity of SnV centers. These results highlight substrate temperature as a key parameter for controlling SnV incorporation during MW PE CVD growth and provide insights into optimizing fabrication strategies for diamond-based quantum technologies.
Tin-Vacancy (Sn-V) colour centres in diamond have a spin coherence time in the millisecond range at temperatures of 2 K, so they are promising to be used in diamond-based quantum optical devices. However, the incorporation of large Sn atoms into a dense diamond lattice is a non-trivial problem. The objective of our work is to use microwave plasma-assisted chemical vapour deposition (CVD) to grow Sn-doped diamond with submicron SnO 2 particles as a solid-state source of impurity. Well-faceted diamond microcrystals with sizes of a few micrometres were formed on AlN substrates. The photoluminescence (PL) signal with zero-phonon line (ZPL) peak for Sn-V centre at ≈620 nm was measured at room temperature (RT) and at 7 K. The peak width (full width at half-maximum) was measured to be 1.1–1.7 nm at RT and ≈0.05 nm at 7 K. The observed variations of ZPL shape and position, in particular, narrowing of PL peak at RT and formation of single-line fine structure at low- T , are attributed to strain in the crystallites. The diamond doping with Sn via CVD process offers a new route to from Sn-V colour centre in the bulk of the diamond crystallites. This article is part of the Theo Murphy meeting issue 'Diamond for quantum applications'.
Quantum emitters in diamond are a promising candidate for quantum network applications. Here, we show basic properties of tin-vacancy (SnV) centers in diamond, which we recently discovered. The SnV center shows a sharp zero phonon line and a high fluorescence intensity. The SnV center has a possibility to have a long spin coherence time in the Kelvin temperature range, in contrast to other group-IV color centers, i.e. silicon-vacancy and germanium-vacancy centers. We discuss important experiments regarding spin and optical properties of the SnV quantum emitter for further development towards quantum network.
Group-IV color centers in diamonds are promising not only as spin-photon interfaces for quantum networks but also as multicolor photoluminescence probes and all-optical temperature sensors for biological research. Therefore, generating group-IV color centers in detonation nanodiamonds (DNDs), the smallest class of diamond nanocrystals, has become a research focal point. This approach holds potential for the noninvasive introduction of diamond sensors into living cell organelles, enabling sensing of local structural and temperature changes with minimal disturbance. Following the successful generation of silicon- and germanium-vacancy centers in DNDs, the generation of tin-vacancy (SnV) centers was investigated. Similar to other group-IV color centers, the SnV centers exhibit strong photoluminescence. In addition, the SnV center offers a long spin coherence time compared with those of silicon- and germanium-vacancy centers. However, the strain induced by large Sn atoms poses substantial challenges for generating SnV centers in ultrasmall nanodiamonds. In this study, Sn-doped DNDs with a mean particle size of ~ 5 nm were subjected to a 3 days boiling acid treatment, which led to sharp zero-phonon lines of SnV centers at ~ 620 nm in the photoluminescence spectra. Photon autocorrelation measurements further revealed the presence of single SnV centers in these DNDs.
Nanodiamonds with color centers have recently become a focus of photonic quantum information technologies. Among the various vacancies in diamonds, Tin vacancy (SnV) centers have promising properties[3], such as high brightness, high emission efficiency (60%) from a zero-phonon line (ZPL) at about 620 nm, lifetime-limited linewidths, and a long coherence time of the electronic spin. A reported method for fabricating nanodiamonds, including SnV centers, is the synthesis by microwave plasma chemical vapor deposition[4]. In this method, inorganic compounds were used to introduce a layer of oxides and chlorides that serve Sn ions. However, this method would be difficult to precisely control both the size of the nanodiamonds and the number of defect centers. Here, we report an alternative approach for creating SnV centers in nanodiamonds using ion implantation. We use type-Ib diamond monocrystalline suspension (MSY 0.05, purchased from Microdiamant). Small amounts of the suspension are spin-coated several times on substrates. Sn ions are implanted into the samples with an energy of 800 KeV and ion fluence of 1014 ions/cm2. We then anneal the implanted samples in a high vacuum for about 20 hours at 1200oC. After annealing, the samples are heated at about 500 degrees to remove the sp2 carbon layer on the surface. Finally, the nanodiamonds are transferred to silica substrates. We use a confocal microscope system for the optical measurement. A continuous-wave laser (λ=520 nm) is used to excite the SnV centers in the nanodiamonds. The laser's excitation power is about 10 mW. The laser beam is focused on the nanodiamonds with an objective lens with a numerical aperture of 0.95. The samples are scanned at a step size of 200 nm using a three-axis piezo actuator. The fluorescence is collected with the same objective lens and measured by a single-photon counting module and a spectrometer.
Group IV color centers in diamond (Si, Ge, Sn, and Pb) have recently emerged as promising candidates for realization of scalable quantum photonics. However, their synthesis in nanoscale diamond is still in its infancy. In this work we demonstrate controlled synthesis of selected group IV defects (Ge and Sn) into nanodiamonds and nanoscale single crystal diamond membranes by microwave plasma chemical vapor deposition. We take advantage of inorganic salts to prepare the chemical precursors that contain the required ions that are then incorporated into the growing diamond. Photoluminescence measurements confirm that the selected group IV emitters are present in the diamond without degrading its structural quality. Our results are important to expand the versatile synthesis of color centers in diamond.
Point defects in diamond, promising candidates for nanoscale pressure- and temperature-sensing applications, are potentially scalable in polycrystalline diamond fabricated using the microwave plasma-enhanced chemical vapor deposition (MW PE CVD) technique. However, this approach introduces residual stress in the diamond films, leading to variations in the characteristic zero phonon line (ZPL) of the point defect in diamond. Here, we report the effect of residual stress on germanium-vacancy (GeV) centers in MW PE CVD nanocrystalline diamond (NCD) films fabricated using single crystal Ge as the substrate and solid dopant source. GeV ensemble formation indicated by the zero phonon line (ZPL) at ∼602 nm is confirmed by room temperature (RT) photoluminescence (PL) measurements. PL mapping results show spatial nonuniformity in GeV formation along with other defects, including silicon-vacancy centers in the diamond films. The residual stress in NCD results in shifts in the PL peak positions. By estimating a stress shift coefficient of (2.9 ± 0.9) nm/GPa, the GeV PL peak position in the NCD film is determined to be between 598.7 and 603.2 nm. A larger ground state splitting due to the strain on a GeV-incorporated NCD pillar at a low temperature (10 K) is also reported. We also report the observation of intense ZPLs at RT that in some cases could be related to low Ge concentration and the surrounding crystalline environment. In addition, we also observe thicker microcrystalline diamond (MCD) films delaminate from the Ge substrate due to film residual stress and graphitic phase at the diamond/Ge substrate interface (confirmed by electron energy loss spectroscopy). Using this approach, a free-standing color center incorporated MCD film with dimensions up to 1 × 1 cm 2 is fabricated. Qualitative analysis using time-of-flight secondary ion mass spectroscopy reveals the presence of impurities, including Ge and silicon, in the MCD film. Our experimental results will provide insights into the scalability of GeV fabrication using the MW PE CVD technique and effectively implement NCD-based nanoscale-sensing applications.