arXiv:2610.04820
Sidewall spacer passivated epitaxial NbN/AlN/NbN Josephson junctions for superconducting qubit applications
Koki Honda, Daiki Kurihara, Hiroki Kutsuma, Hirotaka Terai, Taro Yamashita
Abstract
Epitaxial NbN/AlN/NbN Josephson junctions are promising alternatives to conventional Al/AlO$_x$/Al junctions for superconducting qubits due to their crystalline tunnel barriers and the high transition temperature of NbN. However, their integration into quantum circuits typically requires complex fabrication processes involving amorphous interlayer dielectrics, which can degrade qubit coherence times. To address these issues, we developed sidewall spacer passivated epitaxial NbN/AlN/NbN junctions using a fabrication process that reduces both the volume of amorphous dielectric material and fabrication complexity. The fabricated junctions exhibited a large gap voltage of approximately 5.6 mV and low subgap leakage currents. By varying the thickness of the AlN tunnel barrier, high-quality junctions were fabricated over a wide range of critical current densities ${\it J}_c$, from 0.3 to 10$^4$ A/cm$^2$. In addition, the comparison of the current-voltage characteristics before and after buffered hydrofluoric acid treatment indicated that the wet etching process did not degrade the electrical characteristics of the junctions. These results establish a scalable fabrication process for epitaxial Josephson junctions and provide a promising platform for high-coherence nitride-based superconducting qubits.
AI Summary
Epitaxial NbN/AlN/NbN Josephson junctions offer crystalline tunnel barriers, but their integration typically requires amorphous interlayer dielectrics that can introduce microwave loss. This paper investigates whether a self-aligned sidewall-spacer process, previously used for other trilayer junctions, can simplify fabrication and reduce dielectric volume while preserving NbN/AlN/NbN junction characteristics. The process uses sputtered trilayers on MgO substrates, chlorine-based trilayer etching, PECVD $\mathrm{SiO_2}$ deposition and anisotropic spacer etching, followed by NbN wiring deposition and patterning. DC current–voltage measurements at 2.3 K show gap voltages near 5.6 mV. The subgap-to-normal resistance ratio, evaluated at 3 mV and 10 mV respectively, is approximately 100 for junctions with critical current densities near 1 and 22 $\mathrm{A/cm^2}$, and exceeds 10 near 232 and 1,210 $\mathrm{A/cm^2}$. Varying the AlN barrier thickness gives inferred critical current densities spanning $0.3$–$10^4\,\mathrm{A/cm^2}$, with an exponential thickness dependence corresponding to an estimated barrier height of approximately 1.0 eV. Selected junctions show no significant change in DC characteristics after buffered hydrofluoric acid treatment intended to remove the oxide spacer. The measurements establish DC process compatibility rather than qubit coherence or microwave-loss performance; no qubit measurements are reported. Critical current densities are inferred using the Ambegaokar–Baratoff relation and nominal junction areas because environmental noise and trapped flux complicate direct critical-current measurements. Barrier thicknesses are estimated from deposition rates and times. The paper also notes that MgO substrate loss limited coherence in earlier NbN-based qubits.
Error found: The claim that scalability is established is not backed by fabrication-yield, uniformity, or device-to-device variability measurements, although the simplified process plausibly supports future scaling. Table 1 lists mutually inconsistent values for junction c: its critical current of 64.3 µA and normal resistance of 64.3 Ω imply IcRn = 4.13 mV rather than the reported 3.18 mV.
Written by gpt-6.1-sol from the paper's full text. Automated: it can be wrong.
- Comments
- 9 pages, 4 figures