We report on the fabrication and characterization of superconducting coplanar waveguide (CPW) resonators based on titanium nitride (TiN) thin films deposited on 200\,mm diameter high-resistivity Si(100) substrates. We systematically investigate how deposition conditions, dry-etch power and in-situ resist strip temperature affect morphology, superconducting properties and dielectric losses. By tuning reactive sputtering conditions, three distinct preferred out-of-plane crystal orientations - (111), (200), and a mix of both are achieved. Our results demonstrate that all films exhibit similar minimal two-level system (TLS) losses, with TiN111 exhibiting the lowest median TLS losses
δ~TLS, and greater robustness against reoxidation. The applied structuring process, in contrast, has a far greater influence on the TLS loss than the crystal orientation of the TiN film and, consequently, the intrinsic material properties of the superconducting layer. The lowest TLS losses for all TiN depositions were achieved with a low power etch and low temperature resist strip. An additional buffered oxide etch (BOE) treatment could remove high-loss interfacial oxides at the metal-air (MA) and substrate-air (SA) interface and recover the etch-induced TLS losses. Consequently, TiN resonators exhibiting
δ~TLS values as low as
9.67×10−7 were realized. The corresponding median low-power loss,
δ~LP, amounts to
11.04×10−7, which translates to an internal quality factor approaching one million. These findings highlight the critical role of process induced oxide formation at the MA and SA interfaces in limiting the performance of TiN resonators and provide a scalable, low-loss process compatible with industry-grade 200\,mm CMOS qubit fabrication workflows.
Superconducting qubits are a promising platform for large-scale quantum computing. Besides the Josephson junction, most parts of a superconducting qubit are made of a planar, patterned superconducting thin films. In the past, most qubit architectures have relied on niobium (Nb) as the material of choice for the superconducting layer. However, there is also a variety of alternative materials with potentially less losses, which may thereby result in increased qubit performance. One such material is tantalum (Ta), for which high-performance qubit components have already been demonstrated. In this study, we report the sputter-deposition of Ta thin films directly on heated and unheated silicon (Si) substrates as well as onto different, nanometer-thin seed layers from tantalum nitride (TaN), titanium nitride (TiN) or aluminum nitride (AIN) that were deposited first. The thin films are characterized in terms of surface morphology, crystal structure, phase composition, critical temperature, residual resistance ratio (RRR) and RF-performance. We obtain thin films indicative of pure alpha-Ta for high temperature (600°C) sputtering directly on silicon and for Ta deposited on TaN or TiN seed layers. Coplanar waveguide (CPW) resonator measurements show that the Ta deposited directly on the heated silicon substrate performs best with internal quality factors Qi reaching 1xl06in the single-photon regime, measured at T=100 mK.